9Cr18Mo Peeling and Calender Circle

  Material 9cr18Mo

  Ingredients:

  C Si Mn P S Cr Ni Mo V Cu Nb N

  0.95 to 1.10 ≤0.8 ≤0.8 ≤0.040 0.03 16 to 18 0.6 0.4 to 0.7 is allowed

  Heat treatment regime

  Annealing: 800 ~ 920℃ slow cooling HBW ≤269

  Quenching: 1000 ~ 1050℃ oil cooling

  Tempering: 200 ~ 300℃ oil, air cooling HRC can reach 55

  Standard: GB/T 1220-1992

  ● Characteristics and scope of application:

  Due to the high carbon content in the steel, it has a high hardness and wear resistance after quenching, and has excellent rust and corrosion resistance in the atmosphere, water and some acid and salt aqueous solutions, and it is more obvious when the steel contains molybdenum. It is used to manufacture cutting tools, cutting tools, surgical blades, bearings, valves and other parts that are subjected to high friction and work under corrosive media conditions.


Previous:9cr18mo Rolling Next:9Cr18Mo Zero Cu